Seven measures to reduce defects in mold processing

Release time:2021-08-23

In order to improve the performance of the mold, many manufacturers will process the mold properly. Mold processing refers to the processing of forming and punching tools. In addition, it also includes cutting die and die-cutting die. However, in many cases, the mold is processed. It will also reflect processing defects, resulting in the decline of mold performance. How to establish mold processing defects? The following seven measures can accumulate mold processing defects.


1. Reasonable selection and dressing of grinding wheel


White corundum grinding wheel is better. Its performance is hard and brittle, and it is easy to produce new cutting edges. Therefore, the cutting force is small and the grinding heat is small. Select medium particle size, such as 46 ~ 60 mesh. The hardness of the grinding wheel is medium soft and medium soft (ZR1, Zr2 and R1, R2), that is, coarse-grained, low hardness grinding wheel, good self excitation can reduce the cutting heat.


It is very important to choose a suitable grinding wheel for fine grinding. GD single crystal corundum grinding wheel is more suitable for high vanadium and high molybdenum conditions of die steel. When machining cemented carbide and materials with high quenching hardness, organic bond diamond is preferred. The self grinding performance of grinding wheel and organic bond grinding wheel is good, and the roughness of grinding workpiece can reach Ra0.2 μ m。 In recent years, with the application of new materials, CBN (cubic boron nitride) grinding wheels have shown good machining results. The effect of finish machining on CNC forming grinder, coordinate grinder and CNC Internal and external grinder is better than that of other types of grinding wheels.


In the grinding process, attention should be paid to timely dressing the grinding wheel to keep it sharp. After passivation, the grinding wheel will slip and squeeze on the surface of the workpiece, causing burns on the surface of the workpiece and reducing its strength.


2. Rational use of cooling lubricants


Play the three functions of cooling, flushing and lubrication, keep the cooling and lubrication clean, control the grinding heat within the allowable range, and prevent the thermal deformation of the workpiece. Improve the cooling conditions during grinding, such as using oil immersed grinding wheel or internally cooled grinding wheel. When the cutting fluid is introduced into the center of the grinding wheel, the cutting fluid can directly enter the grinding area, which has an effective cooling effect and prevents the workpiece surface from being burned.


3. Try to reduce the quenching stress after heat treatment


Due to the effect of quenching stress and grinding force, the phase transformation of network carbonized structure is easy to cause workpiece cracks. For high-precision dies, in order to eliminate grinding residual stress, low-temperature aging treatment should be carried out after grinding to improve toughness.


4. Eliminate grinding stress


The mold can also be immersed in a salt bath at 260 ~ 315 ℃ for 1.5 minutes, and then cooled in oil at 30 ℃, which can reduce the hardness by 1hrc and the residual stress by 40% - 65%.


5. Constant temperature grinding


For precision grinding of precision dies with dimensional tolerance within 0.01mm, attention should be paid to the influence of ambient temperature, and constant temperature grinding is required. The calculation shows that for a 300mm long steel, when the temperature difference is 3 ℃, the material will have 10.8 μ Change about M (10.8=1.2 × three × 3. The deformation per 100mm is 1.2 μ M/ ℃), and each finishing process needs to consider the influence of this factor.


6. Electrolytic grinding processing


Improve mold manufacturing accuracy and surface quality. During electrolytic grinding, the grinding wheel scrapes off the oxide film: instead of grinding metal, the grinding force is small, the grinding heat is small, and there will be no grinding burrs, cracks, burns, etc. the surface roughness can generally be better than ra0.16 μ m; In addition, the wear of grinding wheel is small, such as the grinding of cemented carbide. The wear amount of silicon carbide grinding wheel is about 400% - 600% of the weight of cemented carbide being ground. When electrolytic grinding is used, the wear of grinding wheel can only remove 50% - 100% of cemented carbide.


7. Reasonable selection of grinding amount


Fine grinding mode is adopted, with small radial feed and uniform fine grinding. If the radial feed rate and the speed of the grinding wheel are properly reduced and the axial feed rate is increased, the contact area between the grinding wheel and the workpiece can be reduced, the heat dissipation conditions can be improved and the temperature of the workpiece can be increased. The surface can be effectively controlled.

Copyright: Shenzhen Zhongyuan Plastic Co., Ltd. | mold processing customized manufacturer. If you want to know the processing price of the factory, how much is it, and which is good, please contact us Yue ICP Bei No. 17060480
国产精品二区高清在线-91精品91久久久久久| 激情字幕久久久字幕中文-一区二区三区免费黄片| 午夜福利院免费在线观看-久久精品日产第一区二区三区画质| 五月婷婷六月在线观看视频-亚洲黑寡妇黄色一级片| 女主播啪啪大秀免费观看-精品99午夜福利影院| 久久亚州天堂一区二区-色噜噜色哟哟一区二区三区| 亚洲av成人一区国产精品网-国产偷_久久一级精品a免费| 蜜臀一区二区三区精品在线-99久久久精品免费看国产| 少妇一区二区三区粉嫩av-国产精品区久久久久久久| 日韩中文字幕v亚洲中文字幕-日韩亚洲av免费在线观看| 国产高清av免费在线观看-黄片毛片大全一区二区三区| 久久99热这里都是精品啊-国产成人亚洲精品无码aV| 国产剧情av中文字幕-五月婷婷在线手机视频| 人妻日韩精品中文字幕图片-麻豆极度性感诱人在线露脸| 久艹在线观看视频免费-人妻偷人精品一区二区三区| 亚洲黄片三级三级三级-国产成人一区二区在线视频| 性激烈欧美三级在线播放-久久中文字幕人妻少妇| 亚洲欧美日韩国产一区二区三区-国产欧美日韩一区二区免费| 国产一区二区三区四区五区麻豆-欧美一级在线视频播放| 亚洲欧美日韩国产一区二区三区-国产欧美日韩一区二区免费| 久久精品人妻一区二区三区极品-久久99热这里只有精品免费| 18禁真人在线无遮挡羞免费-中文字幕精品一区二区三区四区| 国产欧美日韩精品一区在线-久久精品视频免费获取地址| 日韩亚洲欧美综合在线-成人在线网站在线观看| 国产福利视频一区二区三区-日韩人妻中文视频精品| 免费av一区在线观看-国产精品视频高潮流白浆视频免费| 国产精品v欧美精品v日韩精品-国产欧美日韩精品区一区二污污污| 午夜日韩精品在线视频-亚洲网老鸭窝男人的天堂| 黄片黄片在线免费观看-激情综合网激情五月俺也去| 97人妻精品一区二区三区爱与-日韩精品亚洲专区在线观看| 亚洲欧美激情自拍色图-国产亚洲精品sese在线播放| 日本少妇激情一区二区-亚洲自偷自拍熟女另类蜜臀| 91亚洲美女视频在线-熟妇人妻精品一区二区三区蜜臀| 欧洲精品一区二区三区中文字幕-91久久国产综合久久蜜月精品| 国产小黄片高清在线观看-涩涩鲁精品亚洲一区二区| 国产老熟女激情小视频-成人一区二区人妻不卡视频| 欧美精品一区二区三区爽爽爽-日韩国产精品亚洲经典| 欧美日韩精品人妻在线-在线播放中文字幕一区| 亚洲国产中文欧美一区二区三区-国产精品一区二区视频成人| 亚洲日本一区二区三区黄色电形-中文字幕乱码免费熟女| 在线观看中午中文乱码-2021国产一级在线观看|